Madeira-320AS certified to EN 20471 (Contrast colors)

June 2020, XM FireLine™ fr-fabric Madeira-320 AS in Dark Navy colour has been certified to EN 20471 (Contrast colours). 

Madeira-320 AS is an Antistatic version of our best-selling Madeira-320 pure cotton flame-retardant fabric. Madeira-320 AS is a protective fabric made with antistatic yarn (1%) and cotton (99%). It can be used for welders clothing as well as for different metal processing works in heavy machinery, automotive manufacturing, etc. 

The Standard EN 20471:2013 specifies requirements for high visibility clothing. The high visibility clothing is intended to provide conspicuity of the wearer in any light condition when viewed by operators of vehicles or other mechanized equipment during daylight conditions and under illumination of headlights in the dark.

According to EN 20471, our fr fabric Madeira-320 AS has successfully passed the following tests:

COLOUR FASTNESS TO RUBBING (ISO 105-X12:2016) – performance level PASS

The method is applicable to textiles made from all kinds of fibres in the form of yarn or fabric, including textile floor coverings, whether dyed or printed. Two tests may be made, one with a dry rubbing cloth and one with a wet rubbing cloth.

Immediate Appraisal after Testing

DRY STAINING

  • Wrap: 4-5 – PASS
  • Weft: 4-5 – PASS

The limit set by the Standard EN ISO 20471:2013 + A1:2016 for color fastness to rubbing is 4, in dry.

COLOUR FASTNESS TO PERSPIRATION (EN ISO 105-E04:2013) – performance level PASS

This test is intended to determine the resistance of color of dyed textile to the action of acidic and alkaline perspiration. This criterion does not apply to white products, to products that are neither dyed nor printed, to furniture fabrics, curtains or similar textiles intended for interior decoration.

ALKALINE SOLUTION

  • change in colour: 5 – PASS
    • staining (cotton/wool): 4-5 / 4-5 – PASS

ACID SOLUTION

  • change in colour: 5 – PASS
  • staining (cotton/wool): 4-5 / 4-5 – PASS

The limit set by the Standard EN ISO 20471:2013/A1:2016 point (5.3.2) for testing of colour fastness to perspiration, is 4 for degradation and 4 for staining

 

COLOUR FASTNESS TO DOMESTIC AND COMMERCIAL LAUNDERING (EN ISO 105-C06:2010) – performance level – PASS

specifies a procedure to determine the maximum force and elongation at maximum force of textile fabrics using a strip method.

The method is mainly applicable to woven textile fabrics, including fabrics which exhibit stretch characteristics imparted by the presence of an elastomeric fibre, mechanical, or chemical treatment. It can be applicable to fabrics produced by other techniques. It is not normally applicable to geotextiles, nonwovens, coated fabrics, textile-glass woven fabrics, and fabrics made from carbon fibres or polyolefin tape yarns.

The method specifies the determination of the maximum force and elongation at maximum force of test specimens in equilibrium with the standard atmosphere for testing, and of test specimens in the wet state.

  • change in colour: 5 – PASS
  • staining (cotton/viscose): 4-5 / 4-5 – PASS

The limit set by the Standard EN ISO 20471:2013/A1:2016 point (5.3.3), for testing of colour fastness to dry cleaning, is 4 for staining.

 

DETERMINATION OF BREAKING STRENGTH AND ELONGATION (EN ISO 13934-1:2013) – performance level  PASS

The method is mainly applicable to woven textile fabrics, including fabrics which exhibit stretch characteristics imparted by the presence of an elastomeric fibre, mechanical, or chemical treatment. It can be applicable to fabrics produced by other techniques. It is not normally applicable to geotextiles, nonwovens, coated fabrics, textile-glass woven fabrics, and fabrics made from carbon fibres or polyolefin tape yarns.

The method specifies the determination of the maximum force and elongation at maximum force of test specimens in equilibrium with the standard atmosphere for testing, and of test specimens in the wet state.

The method is restricted to the use of constant rate of extension (CRE) testing machines.

BREAKING STRENGTH

  • Wrap: -1900N – PASS
  • Weft: -860N – PASS

ELONGATION

  • Wrap: -11.5% – PASS
  • Weft: -15.0% – PASS

The relative expanded uncertainty of Tensile strength resistance is ±5% assay value of the measured, for a probability of coverage of 95%.

WATER VAPOUR RESISTANCE (EN ISO 11092:2014)  – performance level – CLASS 3

The application of this measurement technique is restricted to a maximum thermal resistance and water-vapour resistance which depend on the dimensions and construction of the apparatus used (e.g. 2 m2·K/W and 700 m2·Pa/W respectively, for the minimum specifications of the equipment referred to in ISO 11092:2014).

  • Water vapour resistance Ret (m2Pa/W): 4,80 – PASS

According to the requirements of standard EN ISO 20471:2013/A1:2016, water vapour resistance of all layers of the garment shall be in accordance with the following table:

CLASS 1CLASS 2CLASS 3
40 < Ret20 < Ret ≤ 40Ret ≤ 20

 

DETERMINATION OF DIMENSIONAL CHANGE IN DOMESTIC WASHING AND DRYING (EN ISO 5077:2008)  – performance level – PASS

This International Standard specifies a method for the determination of the dimensional change of fabrics, garments or other textile articles when subjected to an appropriate combination of specified washing and dryingprocedures.In the case of textile articles or deformable materials, it is necessary to exercise all possible caution in the interpretation of the results.

  • Lengthwise: -1,0 – PASS
  • Crosswise: -2,5 – PASS

You can find all the certificates and additional information on the product page.

 

 